A while back I posted that after trying E70S-6 filler rod for TIG
welding 4130 steel, that I preferred using S-2 although the S-6 worked fine. I had more parts to weld tonight, and at Bruce Frank's suggestion, I first sanded the copper coating off the rod and then wiped it with acetone. It made a bigger difference than I expected it to, and it looks like the S-6 will now be my preferred filler rod. I had previously tried the same cleaning technique with the S-2 and it didn't seem to make much difference. In case anybody is interested. ---------------------------------------------------- Del Rawlins- Remove _kills_spammers_ to reply via email. Unofficial Bearhawk FAQ website: http://www.rawlinsbrothers.org/bhfaq/ |